A. voltageananan ƙarfin rufin abu
1.1 Formula
Epoxy resin E-44 100
Diluent Dibromophenyl glycidyl ether 20
Harshen wuta antimony trioxide 10
Silin siliki mai aiki 400 raga 200
Mai ba da magani 593 25
Tsarin abinci na 3
1.2 Tsarin samarwa
1.2.1 Dry silicon foda zuwa abun cikin danshi ƙasa da 0.2%
1.2.2 epoara maɓallin epoxy, na sirara, mai walƙiya, da silin ɗin foda zuwa mai sarrafawa a cikin tsari mai zuwa
1.2.3 Tada zafin jiki zuwa 100 ℃, degas cakuda a karkashin -0.1Mpa injin don 30min zuwa daidaito
1.2.4 Cool zuwa ƙasa da 50 ° C, ƙara wakili mai warkarwa, kiyaye zafin zafin bai wuce 50 ° C ba, digas vacuum degree -0.1Mpa, lokacin haɗuwa bai fi 30min ba, sai a shiga aikin jefa simintin
B. Babban ƙarfin lantarki da ƙananan ƙarfin rufin rufi
2.1 Kirkirar abubuwa
Epoxy resin E-44 100
Diluent Dibromophenyl glycidyl ether 20
Harshen wuta antimony trioxide 10
Silin siliki mai aiki 400 raga 300
S101 95 mai ba da magani
DMP-30 mai hanzari
2.2 Tsarin samarwa
2.2.1 Dry silicon foda zuwa abun cikin danshi ƙasa da 0.2%
2.2.2 Yi abubuwa biyu a cikin tsari mai zuwa
Abubuwan haɗin epoxy, mai hanzari, mai jinkirin wuta, silinon foda 200
B wakili mai warkarwa, sirara, silinon foda 100
2.2.3 Abubuwan A an zafafa shi zuwa 80-100 ℃, kuma an cakuda cakuda a ƙarƙashin -0.1Mpa injin don 30min zuwa daidaito
2.2.4 Zafin jiki na ɓangaren B ya tashi zuwa 50 ℃, kuma an cakuda cakuda a ƙarƙashin -0.1Mpa injin don 30min zuwa daidaito
2.2.5 Cool zuwa kasa 50 ℃, kara bangaren A zuwa bangaren B, kiyaye zafin jiki bai wuce 50 ℃, degas vacuum degree -0.1Mpa, hada lokaci 30min, zaka iya shiga zuba.